← Technical resources
Industrial CT

Industrial CT for metal additive manufacturing: porosity, trapped powder, lattices and deviations from CAD

For anyone printing metal by powder bed fusion, DED or binder jetting: which defects CT finds and which it misses, how much titanium, steel, nickel alloy and aluminum the beam gets through, how voxel size depends on part width, how CT compares with metallography, sampling from qualification to production and the parts you save.

3D printed titanium bracket with an internal lattice on the rotary stage of an industrial CT scanner, next to a monitor showing the CT reconstruction of pores and a slice with internal channels

A titanium alloy bracket comes off a laser powder bed fusion machine after an overnight build. The part stands 60 mm tall, built in 40-micrometer layers, so the laser has made some 1,500 passes, and any one of them could have left something behind: a gas pore, a spot where two tracks never fused, a pocket of powder sealed inside a cavity. Dimensional inspection of the outside surfaces passes it. If the specification asks what is inside, the traditional answer is to cut it, polish the section and put it under a microscope. One cut shows one plane, and the part is gone.

Industrial CT changes exactly that step. It reconstructs the whole volume of the printed part, leaves it intact and lets you compare it with the CAD model and with the defect limits in the contract. On metal additive manufacturing, though, it runs into hard physical limits set by the alloy, the thickness the beam has to cross and the size of the part, and those limits are where to start before you order a scan or consider a system of your own. The fundamentals of the technique are in our industrial CT scanning guide. This piece deals only with printed parts.

What stays inside a printed metal part

The reference vocabulary is ISO/ASTM 52900:2021, which divides additive manufacturing into seven process categories. For metals the ones that matter most are powder bed fusion (laser or electron beam), directed energy deposition (DED, with powder or wire) and binder jetting, where powder is glued with a binder and then sintered in a furnace. Each process leaves its own defects, and an inspection plan that treats them all alike ends up measuring the wrong thing.

NIST's literature review of metal additive manufacturing defects by Kim and Moylan, published in 2018 as NIST AMS 100-16, sorts them by origin and by what they mean for nondestructive evaluation. In laser powder bed fusion the most common are three kinds of porosity. Gas pores are nearly spherical and often come from the powder itself or from the shielding gas. Lack of fusion appears when there isn't enough energy to melt each track properly onto the one below, and it leaves irregular, flattened cavities aligned with the layers, often lined with unmelted powder. Keyhole porosity is the opposite case: excess energy digs into the melt pool and traps vapor. Gong and colleagues, writing in Additive Manufacturing in 2014, showed on Ti-6Al-4V samples how moving the parameters out of the process window shifts the part from one kind to the other.

Alongside porosity come cracks, typical of some nickel alloys prone to hot cracking, residual stresses that distort the part when it is cut from the build plate, the roughness of as-built surfaces and powder trapped in closed cavities. The technical report ISO/ASTM TR 52905:2023 catalogs these defect types for powder bed fusion and DED and reviews them against existing nondestructive methods. As a technical report it is informative only: it describes and sets no acceptance limits.

Lack of fusion shows up edge-on and hides in a section

The shape of a defect decides which method finds it. An 80-micrometer gas pore is a simple three-dimensional object, and CT sees it as a dark sphere from any direction. Lack of fusion is often wide and thin. It can spread half a millimeter across the layer plane and open only a few micrometers in the build direction. In a metallographic section cut parallel to the layers it looks like an irregular patch, and in one cut across the layers it looks like a line that is easy to mistake for a polishing scratch.

In CT the same defect shows up when its opening is larger than the noise in the volume. When it is thinner than a voxel its contrast is smeared into the neighboring voxels, and the segmentation threshold starts to matter a great deal. That is the same problem that leads two labs to report two different porosity values for the same part, which we covered separately in the article on CT porosity and segmentation. For a printed part, that means writing the requirement by defect type, because a single porosity percentage treats a harmless spherical pore and a flat lack-of-fusion defect that behaves like a crack as the same thing.

ASTM E3166-20e1, a guide to nondestructive testing of metal additively manufactured aerospace parts after build, gives CT its own section and states plainly that it does not set accept-reject criteria. It also points out that the critical initial flaw size, the one inspection has to be able to find, is defined by whoever does the fatigue and fracture analysis. So the smallest defect to detect is a design number, chosen by neither the CT lab nor the print shop. Without it, a scan produces images to interpret and no basis for accepting or rejecting the part.

Trapped powder, lattices and conformal channels: where CT has no substitute

In powder bed fusion every closed cavity stays full of the powder it was built in. In the conformal cooling channels of a mold insert, in hydraulic manifolds and in heat exchangers that powder has to come out completely, because a compacted plug in a bend narrows the flow section and can break loose in service. In CT, unmelted powder shows up as a gray region of intermediate density, lighter than empty space and darker than solid metal, since the grains leave plenty of gaps between them. You can see it clearly as long as the channel is wide compared with the voxel. A 3 mm channel in an 80 mm insert is straightforward to check, while a 0.8 mm channel in a 200 mm part is at the limit.

Lattice structures are the extreme case. Thousands of struts 0.3 to 1 mm thick, nodes and repeating cells: no probe and no optical scanner reaches inside, and a metallographic section shows ten or so at a time. CT can measure strut thickness against the CAD model, find broken struts or unfused nodes and quantify the sintered powder still stuck to the surfaces, which adds weight and changes stiffness. The review by du Plessis, Yadroitsev, Yadroitsava and Le Roux in 3D Printing and Additive Manufacturing (2018) collects these applications and suggests different scan strategies for research, development and production.

Internal roughness is the last piece. As-built laser-fused surfaces are rough, with partly melted particles stuck to them and steps between layers, and no contact instrument can measure them inside a channel. CT can rebuild their profile, but only with a voxel much smaller than the height of the irregularities. The review by Thompson, Maskery and Leach in Measurement Science and Technology (2016) named resolution in porosity measurement and the lack of research on surface texture measurement as the main barriers to CT in additive manufacturing, and the review by Townsend and colleagues in Precision Engineering (2016) shows how much roughness parameters depend on the method used to measure them. For an internal channel, then, ask for a qualitative check of residues and blockages, and treat roughness as a separate measurement on a sectioned coupon or a small region scanned at high resolution.

How much metal the beam gets through: titanium, steel, nickel alloys and aluminum

CT needs a measurable share of the X-rays to cross the part along every viewing direction. Attenuation rises with material density and atomic number and falls with energy. Using the attenuation coefficients in the NIST tables by Hubbell and Seltzer you can run a simple calculation: the thickness that lets 10% of the beam through at two fixed energies. The 10% threshold is our own working assumption, alloys are approximated by their base metal, and the values apply to single-energy photons.

Material (density used)Thickness at 10% transmission, 150 keVThickness at 10% transmission, 300 keV
Aluminum (2.70 g/cm³)about 62 mmabout 82 mm
Titanium, as Ti-6Al-4V (4.43 g/cm³)about 32 mmabout 50 mm
Steel, calculated as iron (7.9 g/cm³)about 15 mmabout 27 mm
Nickel alloy such as 718, calculated as nickel (8.2 g/cm³)about 13 mmabout 24 mm

At 150 keV, 10 mm of nickel alloy attenuates as much as about 49 mm of aluminum, and in alloy 718 the niobium weighs in even more at low energies. There is also a correction to make when reading kV figures. An X-ray tube emits a continuous spectrum whose mean energy sits well below the peak voltage, and the part itself filters out the softer components. A nickel alloy 718 part with solid walls over 20 mm therefore needs high voltages, often above 300 kV, and a detector that can handle long exposures. Aluminum parts or thin titanium walls, on the other hand, work at the lower voltages of microfocus systems, which have smaller focal spots and better resolution.

That filtering by the part also causes the most troublesome artifact on dense metals, beam hardening, described as early as 1976 by Brooks and Di Chiro. The center of thick sections looks less dense than the edges, and dark streaks appear between two heavy walls that can pass for defects. Metal filters in front of the tube keep it in check, together with software corrections and, on very dense parts, with the fan-beam CT and linear detector described in ASTM E1570-19(2026), which picks up less scattered radiation than the cone-beam geometry covered by ASTM E3375-23, at the cost of longer scan times. For a part the beam barely gets through, the way it sits on the rotary stage matters as much as the kV, because it cuts the longest path through metal.

Have a printed part you want scanned?

Tell us the alloy, process, size and the smallest defect the drawing requires you to find: we'll tell you what resolution that part allows and arrange a trial CT scan, with no obligation. Quote within 24 hours.

Email us Message us on WhatsApp

Part width sets the voxel size

In cone-beam CT the part has to fit almost entirely within the detector's field of view, so the voxel is roughly the object's width divided by the usable pixels. With a 2,000 to 3,000 pixel detector, a 10 mm test cube gets down to a few micrometers, a 60 mm bracket lands around 20 to 30 micrometers and a 250 mm manifold around 100. Laser powder bed fusion powders are typically a few tens of micrometers across, so on the whole manifold a pore the size of a powder grain fills less than one voxel. The method standards, from the ASTM E1441-19(2026) guide to ISO 15708-2:2025 on principles, equipment and samples, describe these relationships and how to verify a system's performance. The voxel count needed to see a pore is worked out in the article on CT for porosity in castings.

That leads to the strategy most metal printing shops use. Witness coupons built on the same plate, cubes or cylinders a few millimeters across, are scanned at high resolution and show how the process behaved in that build. The full part is scanned at a coarser resolution to catch large defects, residual powder and distortion. Where detail is needed, on a critical fillet or a narrow channel, a local scan zooms in on that region only. The combination works well as long as you remember that the coupon stands for the plate and not for the individual part, since a shadow in the gas flow or a poorly designed support stays local.

Comparing the part with CAD: distortion, shrinkage and supports

Residual stresses make the part move when it is cut from the plate and during heat treatment. Thin walls warp, overhangs lift and holes change shape. In binder jetting, sintering adds heavy shrinkage that has to be compensated in the model and makes geometry the first thing to check. A single CT scan returns a map of deviations between the part surface and the CAD model, inside and out, and shows right away whether the distortion follows a repeatable pattern that can be corrected in the build file.

A color map still isn't a measurement. To say a dimension is within tolerance you need surface determination, a verified volume scale and a stated uncertainty for that measuring task, as the VDI/VDE 2630 Part 1.2:2018 guideline on influencing variables in dimensional CT explains. The details are in the article on CT dimensional metrology, and if there is no starting model, the reverse route from part to file is covered in the one on CT reverse engineering. For the same reason NASA-STD-6030, the agency's additive manufacturing requirements for spaceflight systems, allows internal measurements to be confirmed with CT provided a part analog reference is used to check their accuracy and precision.

The geometric capability of the printer itself is also qualified with test pieces. ISO/ASTM 52902:2023 defines a set of standard geometries and the quantities to measure on them but leaves the measurement method open. For internal features such as closed holes or hidden walls, CT is the only method that reaches them without cutting.

What metallography finds and what CT finds

Metallographic sectioning remains irreplaceable for anything about microstructure: phases, grains, melt pool boundaries, the effect of heat treatment and hot isostatic pressing, very tight cracks. Under the microscope resolution drops below one micrometer, and on a polished plane a thin lack-of-fusion defect shows up better than in any CT volume. Its limit is statistical. One section through a bracket built in 1,500 layers looks at a single plane, and the odds that this plane runs through the largest defect in the part are low.

CT looks at the whole volume, tells you where each indication sits relative to the surface and the fillets, and leaves the part available for mechanical testing or delivery. It doesn't see microstructure, can't vouch for defects below its own resolution and gives porosity values that depend on segmentation. In the interlaboratory comparison published by du Plessis, le Roux and colleagues in Additive Manufacturing (2019), ten labs scanned the same three laser-fused Ti-6Al-4V parts. The results support the method, but they also show that comparing quantitative values across labs needs more consistent procedures and image analysis. Archimedes density measurement rounds out the picture with a fast, cheap global density figure that says nothing about where the pores are.

In practice the two methods hand off to each other. CT points to the indications worth a closer look, and the cut goes there, at that location, instead of through a plane picked at random. Nondestructive testing decides where to look. Destructive testing confirms what is there and measures what a scan can't provide, such as mechanical and fatigue properties, for which ASTM E3166 itself refers readers to the ASTM F3122 guide.

From parameter qualification to production: how many scans you need

During parameter development the scans are mostly of small coupons. A plate with 20 to 30 cubes built at different energy settings, scanned at high resolution, shows in a few scans where lack of fusion appears and where keyholing starts, and the cubes stay intact for hardness testing and targeted metallography. In first article qualification, full scans of the first units set a baseline: location and type of the typical defects, deviations from CAD, powder residues. This is when you decide which zones of the part are critical and what resolution to require in production.

In production, sampling depends on criticality. NASA-STD-6030 sorts parts into Classes A, B and C by consequence of failure, with subclasses that account for structural demand and process risk, and ties the required controls to the class. Outside aerospace the same logic goes into the contract between customer and supplier. A part whose failure would stop a plant or put people at risk justifies 100% CT, at least on the critical zones. A structural part with comfortable margins can rely on witness coupons for every plate plus a full scan on a sample basis, for example one part per lot or per powder change. The plan should be written before production starts, with the smallest defect to detect and the rule for counting pores, and not after the first reject.

Counting the parts you don't cut

The economic value of CT on additive parts comes down to three items, and none of them needs bold assumptions. The first is the parts you keep. If a plate holds ten brackets and qualification calls for two in metallography, 20% of the first production run becomes scrap, along with the machine hours, powder and downstream machining built into it. With CT those two brackets stay available, and cutting is limited to cases where the scan finds something worth investigating.

The second is qualification time. A development cycle that waits on cutting, mounting and polishing after every parameter change adds days per iteration, while a scan of the coupons answers for the whole volume, in a time that depends on the application and without using up the coupons. The third is late scrap. A lack-of-fusion defect next to a fillet, found after machining, after hot isostatic pressing or at the customer's acceptance test, costs all the value added up to that point. Finding it on the as-built part costs one scan. These are our own estimates and the numbers shift from part to part, but the order of the three items holds for most printed metal parts.

Once scans run into dozens a week, an outside service gives way to an in-house system. A custom industrial CT system is sized on the densest alloy, the largest part and the resolution the coupons require, not on a catalog sheet. Before getting there it almost always pays to go through an industrial CT scanning service, which shows on real parts which settings you need. Some of the requests we receive are collected in our case studies from real requests, and the full picture of the technology is on the page about industrial computed tomography.

What to send us for an assessment

To tell you what resolution your printed part allows and how to set up the scan, we need a few details:

  • process (laser or electron beam powder bed fusion, DED, binder jetting) and alloy;
  • overall part dimensions and the thickest section of solid metal;
  • critical zones, internal channels or lattices to inspect, with the CAD file if available;
  • smallest defect to detect or the porosity requirement in your specification;
  • project stage (parameter development, first article, production) and number of parts or coupons;
  • treatments already done, such as stress relief or hot isostatic pressing.

You can send them by email to info@dipitech.com or on WhatsApp, with drawings or photos attached. You can also use the contact form.

On a printed metal part the starting point is the smallest defect inspection has to find, and in which zone. Once that number exists, alloy and size tell you whether a scan reaches it on the whole part or only on a coupon, and the inspection plan follows from there. With those details we help you choose between outsourced scanning and a dedicated system, with a quote within 24 hours and technical support in Italy.

Request a quote

Leave your name, email, and a few lines about your application, with no obligation. We reply within 24 hours with initial technical guidance and a quote.

We use your details only to answer this request (privacy notice).

Frequently asked questions about CT for metal additive manufacturing

Which defects does CT find in metal printed parts?

It finds gas pores, lack of fusion between layers, keyhole porosity, unmelted powder left in channels and closed cavities, broken struts in lattice structures and geometric deviations from CAD. The limit is resolution: defects smaller than two or three voxels, or very tight lack-of-fusion defects, can be missed.

What resolution can you get on an additively manufactured part?

It depends mainly on part width: the voxel is roughly the object size divided by the usable detector pixels. With 2,000 to 3,000 pixels a 10 mm cube gets down to a few micrometers, a 60 mm bracket to about 20 to 30 micrometers and a 250 mm manifold to about 100 micrometers.

Can printed nickel alloy 718 or steel parts be CT scanned?

Yes, but the thickness the beam can cross is much lower than in aluminum or titanium. At 150 keV, 10 mm of nickel alloy attenuates as much as about 49 mm of aluminum, so solid walls over 20 mm need high voltages, often above 300 kV, and care with beam hardening artifacts.

Does CT replace metallography on printed parts?

No. Metallography is still needed for microstructure, phases, melt pool boundaries and very tight cracks. CT looks at the whole volume without destroying the part and shows where to cut, so sections are made at the indications it finds rather than through a plane picked at random.

How does trapped powder show up in conformal channels?

In CT, unmelted powder appears as a gray region of intermediate density between empty space and solid metal. It is easy to recognize when the channel is wide compared with the voxel, such as a 3 mm channel in an 80 mm insert, while sub-millimeter channels in large parts are at the limit.

How do I request a trial CT scan of a printed part?

We need the process and alloy, dimensions and thickest solid section, critical zones with the CAD file if available, the smallest defect to detect and the project stage. With those details DIPITECH tells you what resolution you can get, arranges a trial CT scan and prepares a quote within 24 hours.

Sources and references

Related resources

Have printed metal parts to inspect?

Talk to a DIPITECH technical contact: we help you choose between an outsourced CT scanning service and a custom CT system, with a reply within 24 hours and no obligation.

WhatsApp